How to control the quality during the finishing process of cashmere scarves(2)

May 08, 2024

Leave a message

2 ear mark problem

Fringe marks refer to the marks caused by the squeezing of the fringe of the scarf or shawl against the suede surface when the cashmere scarf is steamed during the finishing process. Steaming is the main process that produces ear marks. Generally, scarf fabrics are steamed twice, and can be adjusted according to specific conditions.

2.1 The influence of steaming machine on ear marks

Steaming machine models include N711, MB441 and WPF-98. The first two types are called old steaming machines, and the latter are called new steaming machines. There are obvious differences between the two in terms of producing ear marks. Analysis and research from aspects such as steaming drum, cooling system, tension adjustment, etc. will help solve the problem of ear marks.

2.1.1 Material of steaming roller

The large cylinder drum of the old steamer is made of purple gold copper, and the mesh diameter of the steam outlet holes on the drum is only 4 mm. Because it is made of copper, it is easily oxidized and corroded, clogging the already small holes. The large cylinder drum of the new steamer is made of stainless steel, so there is no corrosion problem, and the diameter of the steam outlet mesh is much larger than that of the old steamer. machine, so the steam inlet and outlet roads are smooth, which enhances the steaming effect.

2.1.2 Steaming time

The old steamed cloth machine steams 3 pieces of cloth, and the steaming time takes 15 minutes; the new steamed cloth machine steams 6 pieces of cloth (same variety), and achieves the same effect, and the steaming time only takes 10 minutes. For plain and dark products, old steaming machines are more likely to produce fringe marks due to the longer steaming time. The uniformity of the inner and outer layers is also affected. Black and brown exported pure wool women's cloths were used to compare the color differences of steamed cloths on new and old cloth steaming machines. On the old steamer, there is a serious color difference between the head of the first horse and the tail of the third horse, which is much larger than the color difference between the head of the first horse and the tail of the sixth horse on the new steamer, which is 450 m apart.

After testing, when the steam supply pressure of the old steamer is 205.8 Pa (2 kg/cm2), the temperature of the inner layer of fabric can reach 100~110℃, but the temperature of the outer layer is only 80~90℃.

2.1.3 Tension device

The tension device is an important factor in the production of scarf fringe marks. The tension device can control the tension of the wrapping cloth during the entire winding process under different conditions according to the winding diameter of the steam roller. From the inside to the outside, from beginning to end, it is uniform and constant, so that the wrapping cloth is always in a flat state, thus Ensure that the fabric does not produce tassel marks, steamed cloth printing and other defects. New steaming machines have this device.

2.2 Solution to the problem of ear marks

①Adjust the working status of the steaming roller so that it is always rotating, which can significantly improve the steaming marks. ② The installed capacity should be reasonably controlled so as to avoid wasting space and not causing tassel marks due to mutual extrusion. ③ The method of double wrapping can significantly change the pressure on the fabric and reduce the pressure. This is very effective in reducing ear marks. ④ Improve the penetration ability of steam and reduce the steaming time, which can reduce the occurrence of ear marks. ⑤When winding the scarf, the fringes of the upper layer and the lower layer should correspond to avoid fringe marks.